(888) 722-8260 | sales@diversifiedbronze.com | Cart
Custom Machining View Capabilities →

C48200

Naval Brass, Medium Leaded

Copper-Zinc Alloys Wrought

Naval brass with a lead addition for improved machinability. The tin content gives dezincification resistance in seawater service.

Tensile Strength
56–75 ksi
Yield Strength
25–53 ksi
Machinability
50 / 100
Density
0.305 lb/in³

Chemical Composition

Element Min % Max %
Copper (Cu) 59 62
Zinc (Zn) Remainder
Tin (Sn) 0.5 1
Lead (Pb) 0.4 1
Iron (Fe) 0.1

Physical Properties

Density 0.305 lb/cu in
Specific Gravity 8.44
Melting Point (Solidus) 1630°F
Melting Point (Liquidus) 1650°F
Electrical Conductivity 26% IACS

Mechanical Properties

Tensile Strength 56–75 ksi
Yield Strength 25–53 ksi
Elongation 15–43%
Hardness 55–80 Rockwell B
Machinability Rating 50

Thermal Properties

Thermal Conductivity 67 Btu/ft·hr·°F
Coefficient of Expansion 11.8 × 10⁻⁶ /°F
Specific Heat 0.09 Btu/lb·°F

Fabrication Properties

Soldering Excellent
Brazing Good
Oxyacetylene Welding Fair
Gas Shielded Arc Fair
Coated Metal Arc Fair
Cold Working Fair
Hot Forming Excellent

Typical Applications

  • Marine hardware
  • Valve stems
  • Screw machine products
  • Fittings and fasteners
  • Condenser plates
  • Pump shafts

Applicable Specifications

  • ASTM B21
  • SAE J461
  • SAE J463